Burn marks in injection molding are surface defects caused by excessive heat when trapped air or gases become compressed inside the mold cavity. They appear as brown or black discolorations, often near the end of the flow path. Severe cases may cause carbonization, making parts unacceptable. Understanding their causes and identifying these defects early helps prevent quality issues during production.
The causes of burn marks are primarily related to the mold and the injection molding process; below, we will analyze these aspects.
Issue with Mold Design
Burn marks in injection moulding parts can be caused by trapped air in the mold cavities. This air is unable to escape at the end of the flow path due to poor mold venting. The trapped air within the mold cavity compresses during injection, generating high temperatures and resulting in burn marks on the finished product.
To prevent burn marks, proper mold design is essential. First, incorporating effective venting systems allows trapped air to escape, reducing the risk of overheating. Additionally, adjusting the gate location, such as placing it closer to the end of the fill or using multiple gates, can optimize the flow path. It helps prevent air from being pushed into areas where it cannot escape easily. Enlarging the gate size can help direct the plastic flow more evenly and give trapped air a better chance to escape through the vents, reducing air compression and the risk of burn marks.
Issue with Injection Speed
Injection molding burn marks occur when the injection speed is too high during molding, particularly at the end of the process. This rapid speed compresses trapped air inside the mold, leading to overheating and ignition, which scorches the plastic and leaves carbon residue.
Reducing the injection speed, especially in the final stages of filling, is a practical solution. It allows trapped air enough time to escape, minimizing the risk of compression and overheating. For thin-walled products, which are particularly susceptible to this defect due to their limited thickness and potential for restricted airflow, using cavity vacuum devices can help ensure gas is effectively removed.
Issue with Mold Temperature and Material Degradation
Excessively high mold temperatures can affect how molten plastic cools and increase the risk of material degradation. When the mold temperature exceeds the recommended range for the selected material, prolonged heat exposure may cause plastic discoloration and thermal degradation. Uneven mold temperatures can also result in inconsistent cooling, creating localized hot spots that contribute to surface defects and burn marks.
To prevent these issues, maintain the mold temperature within the recommended processing range for the selected plastic material. Proper temperature control helps avoid excessive heat buildup, supports consistent cooling, and reduces the risk of material degradation. Regularly monitoring temperature variations across the mold cavity also helps identify hot spots before they affect part quality.
How To Detect Burn Marks?
Detecting burn marks early in the production cycle is crucial to minimizing scrap rates and ensuring consistent product quality. Since burn marks are primarily surface-level appearance defects, they are typically identified through a combination of visual, tactile, and targeted inspection methods:
Visual Inspection Under Proper Lighting
The most effective way to detect burn marks is through careful visual inspection under high-intensity LED lighting. Inspectors look for color gradients ranging from slight yellowing or brownish tints to severe black, charred spots. While slight yellowing might be acceptable for internal or non-cosmetic parts, any sign of black carbonization immediately disqualifies the part.
Tactile Examination
In some cases, especially with minor burns, the defect is easier to feel than to see. Running a gloved finger lightly over the surface can reveal texture anomalies. Burn marks often feel slightly rough, pitted, or raised compared to the smooth, uniform finish of the surrounding healthy plastic.
Magnification and Micro-Inspection
For high-precision components, transparent/translucent plastics, or strict cosmetic surfaces, naked-eye inspection may not be enough. Using magnifying glasses, digital microscopes, or Automated Optical Inspection (AOI) systems helps detect micro-burn marks or subtle discolorations that could compromise aesthetic standards.
Targeting High-Risk Locations
Burn marks rarely appear randomly; they follow the flow of the plastic. It is important to focus on specific “air trap zones”. These include the farthest points from the injection gate (the end of the flow path), blind corners, sharp internal angles, and areas adjacent to parting lines, vents, or ejector pins.
Case Study-How to Get Rid of Burn Marks on Plastic
The following is a practical case study conducted by the Erye engineering team, which explains in detail how we get rid of burn marks on plastic.
Project Introduction
The picture is a plastic burn mark example. The product is a type of connector made of PBT material with a thick wall thickness; the surface is sub-exterior. Our customer has strict quality standards, so it is not allowed to have an appearance defect.
The following are the molding conditions,
| Parameter | Value |
|---|---|
| Mold Temperature | 60~80℃ |
| Material Temperature | 240~260℃ |
| Injection Speed | First stage: 180mm/s; Seconde stage: 135 mm/s; Third stage: 40mm/s |
| Injection Pressure | 1300~1500kgf/cm2 |
| Injection Time | 1.5~3s |
How Do We Fix Burn Marks on Plastic Parts
Cause Analysis
During the initial trial molding process, our engineer analyzed the runner plate and discovered that the burn marks on the plastic are located at the weld line at the end of the product. Our further analysis concluded that the air is unable to vent from the mold cavity, resulting in trapped air and burning.
Solutions
At this stage, our client has confirmed that both the product and mold structure cannot be changed. To address the burn mark issue, engineers can only make adjustments in terms of mold venting and the injection molding process. Our engineers implemented the following solutions:
- Enlarged the venting slots in the mold runner, parting line, and ejector pin areas as much as possible to reduce the amount of end venting, thereby eliminating the burn marks on the plastic.
- Adjusted the injection molding process to multi-stage injection. Due to the product’s thick wall thickness, the last two stages of injection were performed at low or even lower speeds to reduce burn marks.
By combining the above two methods, we effectively improved the burn marks and met the client’s high-quality requirements.
Conclusion
Burn marks are a common injection molding defect. There are many factors that can cause plastic defects, they can be effectively solved by eliminating them parameter by parameter. If you have trouble with burn mark troubleshooting, our experts at Erye Molding are willing to help. Contact us today for help!